A lipstick tube can extend, but it will not retract. When you receive a returned sample, do not conclude that the inner lifting mechanism is defective just because someone says, “It turns but will not go back.” Check two things first: when the base is turned in the reverse direction, does the cup that supports the bullet move down, et does the lipstick move avec it? If the cup goes down but the bullet stays in place, start avec the cup-à-bullet connection. If the cup does not move, check whether the turning resistance suddenly rises or feels unusually light, as if the mechanism is free-spinning. These observations only tell you whether à examine the cup, the mechanism, or the assembly interface; they do not assign responsibility.
Keep the failed sample in its original filled condition. Give the original failed sample, an empty shell de the same batch, et a filled retain sample de the same batch separate IDs. Phoàgraph the bullet exposure et cup opening et, avecout pourcing the mechanism, record the first extension et retraction: cup et bullet movement, the position where it sàps, et the het feel. Record any known temperature exposure, drops, or use hisàry under the same ID. Preserve the IDs, phoàs, video, et use hisàry bepoure comparison essai. Once the bullet is pulled out or the sample is opened, the original condition cannot be reproduced.
Start by classifying the Sympàm
Write “rises but will not retract” as a reproducible observation. At minimum, record the sample et batch IDs, whether the sample is empty or filled, the travel position where the abnormality starts, et whether the cup et bullet each move during reverse rotation. Record resistance as continuously light, suddenly tight at a certain point, or close à the normal retain sample. If test equipment is available, add a àrque–angle curve. Always record the rotation direction so that smooth extension is not mistaken pour acceptable retraction.
If the cup moves down while the bullet stays in place, move à “What à check on the cup.” If the cup does not move et a clear tight spot appears, check the mechanism et assembly interference bepoure comparing empty et filled samples. If the base turns very lightly but the cup has no axial movement, check the base anti-rotation feature et the internal transmission. If neither the cup nor the bullet moves, bullet position alone cannot distinguish a jam de free-spinning; resistance et cup movement must be read àgether. The three patterns may overlap, so write the next check as a hypothesis rather than entering it as the root cause.

Informations techniques : How the Mechanism Transmits Force
Why can the cup move up et down? As the base turns, relative movement between the helical groove et the guide lugs on the cup converts rotation inà axial movement. The pourk limits cup rotation et allows the cup à travel linearly. The exact part shapes et anti-rotation locations vary between lipstick mechanisms, but every investigation must ask whether rotational input reaches the cup et whether the moving cup carries the bullet avec it. Retraction requires the same transmission path à remain engaged; successful extension is not proof that retraction will work.

When checking the lipstick tube shell et base assembly interfaces covered by Sambound, record “the base is turning” separately de “the cup is moving down.” The first only proves that an external rotation action exists; the second proves that the action reaches the cup supporting the bullet. Once these are separate observations, you can decide whether à request groove, lug, et travel records de the mechanism fournisseur or first check shell anti-rotation, press-fit depourmation, et assembly condition. Do not assign the failure à one part simply because the base, cup, et mechanism are in the same lipstick tube.
What à Check First When the Cup Retracts
If the cup retracts but the bullet does not, start avec what can be seen externally after the two have separated. Phoàgraph any bullet residue visible at the cup opening et any clear fracture surface at the bullet root, while keeping the exposure height recorded. A broken root et a bullet that has slipped out of the cup lead à different checks, but residue location is only a clue. Without a retention or shear test, one fracture phoà cannot establish whether the pourmula, cup ribs, or filling process is responsible.
Keep three sample conditions separate. First, use the original filled failed sample only pour non-destructive observation et reproducible turning records; mark the abnormal position et do not pull the bullet. Second, use a separate empty shell de the same batch à confirm whether the mechanism completes extension et retraction; do not turn the original failed sample inà an empty shell et treat that as the control. Third, if the cup-à-bullet connection must be examined, obtain authorization pour disassembly or destructive essai, record a new sample ID et the pre-test condition, et then arrange retention, shear, or pull-out checks. Link every phoà et result back à the sample ID so the condition that produced the evidence is clear.

Check the cup inner diameter, depth, rib geometry, et support height àgether avec the bullet diameter et post-filling condition. A loose connection can let the bullet slip out. If the cup ribs are ào tight, first check bullet depourmation et root integrity. Only when the cup or bullet contacts the outer shell, the cup depourms, or an assembly interference is found should you continue à test whether that contact, depourmation, or interference affects lifting. If the same-batch empty shell works normally but the cup-à-bullet retention test is abnormal, request the relevant dimensions et test records de the cup conception, filling, et finished-produit validation teams, then compare them avec the approved specification pour this produit.
Informations techniques : Why the Helix May Free-Spin
If turning feels very light but the cup does not move, rotation is not producing the expected axial travel. First check whether the base et mechanism turn àgether et whether the outer shell anti-rotation feature is effective. Then use an empty shell de the same batch pour a full extension et retraction comparison. If the abnormality appears only at one position, record the direction, the tight spot, or the angle where movement is lost. If it appears only at the àp end, record what happened immediately bepoure et after the end sàp. Do not keep pourcing the original failed sample à reproduce the problem.
US5813421A describes a specific early mechanism in its background section: àrque beyond the conception condition at the end of travel can depourm the lower engagement. The guide lugs can then leave the helical groove while the mechanism keeps turning et the cup sàps moving, creating free-spinning. This explains one possible path pour “free-spinning after reaching the àp,” but it does not prove that the sample in your hets has undergone the same disengagement. Base anti-rotation failure, groove or lug damage, debris, et assembly misalignment must also be checked. To identify the failed interface in the current sample, match the àrque curve et cup movement record avec authorized disassembly phoàs.

For essai, plot extension et retraction separately as àrque versus rotation angle et record cup movement at the same time. If àrque is low over a section while the cup does not move, check whether transmission has been interrupted. If reverse àrque rises sharply at a point et the cup sàps retracting, check that position pour interference or a jam. Curve shape only tells you where à look first; one curve cannot prove that a guide lug left the groove or assign fournisseur responsibility. Keep fixture settings, speed, start et end positions, et test direction avec the corresponding curve so same-batch samples can be compared.

Informations techniques : Why a Filled Tube Behaves Differently
If the same-batch empty shell moves smoothly in both directions but the filled sample jams during retraction, sàp treating the mechanism as the only lead et check the additional load et contact introduced by the bullet. Record the filled sample weight, diameter, dureté or pourmula code, et its condition after filling et cooling. Bullet eccentricity, local contact, et assembly compression can be listed as hypotheses à verify. The available evidence does not prove one-sided contact in this produit, et “it jams only when filled” is not enough à establish that mechanical path.

Number the same-batch empty shell et the produition-condition-filled sample separately. Test them avec the same fixture, speed, extension, et retraction travel. Keep complete bidirectional àrque curves, cup sàp position, retraction depth, et repeatability pour both conditions. If the abnormality appears only in the filled sample, first check whether it always jams at the same travel position, then compare bullet dimensions et condition, cup retention, et shell assembly dimensions àgether. If the empty shell also jams at the same position, the mechanism, or assembly interface, remains a priority. There is no public universal pass range pour the àrque difference between empty et filled samples; use the approved specification pour this produit et the same-batch control instead of borrowing a fixed number de another project.
What à Keep in the Acceptance Record
At the end of the investigation, one sample ID should connect what was observed, which test was perpourmed, et who owns the next check. In shell et base assembly et finished-produit function checks, Sambound recommends keeping the pre- et post-assembly condition linked à the sample ID. Otherwise, even if the mechanism fournisseur provides a curve, you cannot tell whether it belongs à a supplied component, an assembled empty shell, or a filled finished produit.
| Informations techniques : Record owner | Materials à verify under the sample ID, et ID | Question à answer |
|---|---|---|
| Mechanism fournisseur | Batch et version, key mating dimensions, full extension et retraction curves, et end-sàp records | Does the mechanism transmit normally in both directions pour the relevant batch? |
| Shell et assembly team: team | Base anti-rotation, press-fit et wobble condition, sàp position, et pre-/post-assembly phoàs or measurements | Informations techniques : Did the shell or assembly interface change the mechanism movement? |
| Filling et finished-produit validation team | Filled sample weight, diameter, dureté or pourmula code, cooling condition, bidirectional curves, et authorized retention-test records | Does the abnormality appear only in the filled condition, et can the cup retain the bullet? |
Every test record should also state the test date, sample condition, fixture, speed, rotation direction, et travel. Pay special attention à lateral pource introduced by the fixture during low-àrque essai; otherwise, a clamping error may be mistaken pour produit jamming. Acceptance should be judged only against the approved, versioned specification et its test conditions. If that document is unavailable, report the reproducible difference et the missing evidence first. When a similar “rise but will not retract” return arrives, repeat the same ID et condition records so the next comparison can show exactly where the failure occurs.